Prepared by: Assistant Lecturer Ahmed Saeed Hakim, College of Engineering, Department of Civil Engineering
Abstract
Cracking is one of the most common defects in concrete structures, affecting durability, appearance, and serviceability. It is especially prominent in large-dimension elements, such as mass concrete (e.g., dams, thick foundations, and massive piers) and large floor slabs (e.g., warehouse, factory, and parking floors). This article examines the physical and chemical causes of cracking resulting from shrinkage and temperature changes, explains how restrained stresses develop, and reviews the most important design and construction measures for limiting this phenomenon.
Keywords: cracking, shrinkage, thermal expansion, mass concrete, concrete floors, heat of hydration, contraction joints.
1. Introduction
Concrete is strong in compression, but its tensile strength is limited, generally not exceeding about 8–15% of its compressive strength. When concrete undergoes volume changes, whether due to moisture loss or temperature variation, and these changes are restrained by the soil, adjacent elements, or the inner layers of the element itself, tensile stresses develop that may exceed the concrete's capacity, resulting in cracking (Neville, 2011; Mehta & Monteiro, 2014).
Cracks do not necessarily indicate structural deficiency, but they allow water, chlorides, and sulfates to enter, accelerate corrosion of steel reinforcement, reduce the effectiveness of waterproofing, and affect the serviceability of floors (ACI 224R).
2. Fundamental Mechanisms of Volume Change
2.1 Shrinkage
Shrinkage in concrete takes several forms:
Plastic Shrinkage: Occurs in the first hours before setting, when surface water evaporates faster than bleed water can rise to replace it. It increases in hot, dry, and windy conditions (ACI 305R).
Autogenous Shrinkage: Results from internal consumption of water in the hydration reactions. It is more significant in concrete with a low water-to-cement ratio and in high-performance concrete (Holt, 2001).
Drying Shrinkage: Results from the loss of water held in capillary pores after hardening, and develops over months and years. Its typical value lies in the range of 400–800 microstrain, depending on the mix components and environmental conditions (Neville, 2011).
2.2 Thermal Changes
Concrete expands when heated and contracts when cooled. Its coefficient of thermal expansion is about 10×10⁻⁶ per °C (generally ranging between 7 and 13×10⁻⁶ depending on the aggregate type). Thermal changes arise from two sources:
Heat of hydration: Cement reactions are exothermic. In thick elements, this heat accumulates in the core because of the low thermal conductivity of concrete, causing a substantial rise in internal temperature.
Climatic conditions: Day–night temperature differences and direct sun exposure, which are particularly important in hot climates.
2.3 Restrained Stress
Volume change alone does not cause cracking; freely moving concrete does not crack from shrinkage or expansion. Damage occurs when this movement is restrained. Tensile stresses develop when the restrained strains exceed the concrete's tensile strain capacity, which is relatively small, generally between 100 and 150 microstrain at early ages (Bažant & Najjar, 1972; ACI 207.2R). The level of risk is affected by the degree of restraint, the modulus of elasticity, the creep of concrete (which relieves part of the stress), and the age of the concrete when the stress develops.
3. Cracking in Mass Concrete
Mass concrete is defined as any volume of concrete large enough to require measures to deal with the heat of hydration and the accompanying volume changes, in order to minimize cracking (ACI 207.1R).
3.1 Cracking Mechanism
After placement, the temperature of the element's core rises considerably, while the surface quickly loses heat to the surrounding environment. This gives rise to two patterns of risk:
Cracking due to internal temperature differential: When the hot core expands and is restrained by the cooler surface, tensile stresses develop at the surface and may cause early surface cracking.
Cracking due to subsequent cooling: When the element returns to thermal equilibrium with its surroundings, its entire volume contracts. If the element is restrained by the foundation or by adjacent older pours, through-section cracks develop.
Risks are higher in retaining walls and thick slabs cast on rigid foundations or over older concrete, owing to the high degree of restraint at the interface.
3.2 Influencing Factors
Cement content, type, and heat of hydration.
Element dimensions: the greater the thickness, the slower the heat dissipation.
Concrete temperature at placement and ambient temperature.
Rate of concrete placement and layer thickness.
Aggregate properties, especially its coefficient of thermal expansion.
Restraint conditions and curing practices.
3.3 Control Measures
Mix design: Use low-heat cement, replace part of the cement with supplementary cementitious materials such as fly ash or ground granulated slag, reduce cement content, and select aggregate with a low coefficient of thermal expansion (ACI 207.1R; ACI 207.2R).
Pre-cooling: Cool the ingredients, use ice in place of part of the mixing water, or cool the aggregate to reduce the placing temperature.
Post-cooling: Circulate cold water through embedded pipes within the mass, a method widely used in large dams.
Placement control: Place concrete in layers, delay the next layer to allow heat to dissipate, and divide the mass into sections separated by construction joints.
Insulation and curing: Use thermal insulation or tarpaulins to reduce the core–surface temperature difference, and avoid removing insulation too quickly.
Thermal monitoring: Install temperature sensors inside the mass and monitor them continuously. ACI 301 typically sets reference limits, including a maximum concrete temperature of about 70°C and a core–surface temperature difference of no more than about 20°C, unless analysis or testing demonstrates that other limits are acceptable.
Thermal-structural analysis: Perform numerical simulation at the design stage to predict the development of temperature and stresses.
4. Cracking in Large Floor Slabs
4.1 Cracking Mechanism
Large floors are usually constructed as slabs on ground, in which the concrete is subject to drying shrinkage and thermal contraction simultaneously. Friction between the slab and the subbase restrains horizontal movement, producing tensile stresses. In addition, the top surface dries faster than the bottom, creating a shrinkage differential through the thickness, so the slab tends to curl at the edges and corners, and additional stresses develop under loads.
4.2 Common Cracking Patterns
Plastic cracks: Short surface cracks that appear in the first hours.
Random shrinkage cracks: Longer cracks caused by the absence of joints, excessive joint spacing, or delayed saw-cutting.
Re-entrant corner cracks: Around columns, openings, and manholes due to stress concentration.
Curling-related cracks: At joints and edges.
4.3 Control Measures
Contraction joints: Cut to a depth of about one quarter of the slab thickness (or not less than 25 mm when using conventional saws) to direct cracking into planned lines. It is recommended to cut them early, once the concrete has hardened sufficiently, usually within 4–12 hours depending on conditions, before random cracking occurs (ACI 302.1R).
Joint spacing: Practical guidelines suggest that spacing be proportional to slab thickness (about 24–36 times the thickness for unreinforced slabs), keeping panel shapes close to square and avoiding elongated proportions (ACI 302.1R; ACI 360R).
Isolation joints: Around columns, walls, and fixed structures to allow the slab to move independently.
Subbase: Prepare a uniform and even base, reduce friction where necessary, and control its moisture before placement.
Mix design: Specify a suitable water-to-cement ratio, avoid adding water on site, reduce total water content, and use well-graded aggregate with an appropriate maximum size. Shrinkage-reducing admixtures or fibers may be used when needed.
Construction and curing: Protect the surface from rapid evaporation by applying curing compounds, wet coverings, or vapor barriers in hot and dry conditions, and begin curing immediately after finishing.
Reinforcement: Reinforcement generally does not prevent cracking, but it limits crack widths and keeps the cracked pieces tied together. Shrinkage-compensating concrete or post-tensioned slabs may be adopted for very large floors.
5. Brief Comparison of the Two Cases
Both cases are similar in that restraint is the necessary condition for cracking, but they differ in the dominant cause. In mass concrete, the thermal effect from hydration is the most critical factor, and its control depends on heat management. In large floor slabs, drying shrinkage and ground restraint are the most critical, and their control depends on joints, mix quality, and proper curing.
6. Practical Recommendations
Address crack control at the design stage rather than leaving it to construction.
Prepare a written placement and curing plan suited to the local climate, especially in hot weather.
Monitor temperature continuously in mass elements, and document joint locations and cutting times in floors.
Provide good training and site supervision, since cracking often results from errors in construction and curing rather than from design deficiencies.
Carry out appropriate repair of visible cracks after assessing their causes and effectiveness (ACI 224.1R).
7. Conclusion
Cracking caused by shrinkage and thermal expansion is an expected phenomenon in concrete, and an engineer's ability to control it depends on understanding the restraint mechanism and its effect on stress development. This is achieved through the integration of four aspects: suitable mix design, good planning of joints and element segmentation, thermal management in mass elements, and early, consistent curing. In this way, harmful cracking can be reduced and the durability and service life of structures improved.
References
ACI Committee 207. ACI 207.1R: Guide to Mass Concrete. American Concrete Institute.
ACI Committee 207. ACI 207.2R: Report on Thermal and Volume Change Effects on Cracking of Mass Concrete. American Concrete Institute.
ACI Committee 224. ACI 224R: Control of Cracking in Concrete Structures. American Concrete Institute.
ACI Committee 224. ACI 224.1R: Causes, Evaluation, and Repair of Cracks in Concrete Structures. American Concrete Institute.
ACI Committee 302. ACI 302.1R: Guide to Concrete Floor and Slab Construction. American Concrete Institute.
ACI Committee 360. ACI 360R: Guide to Design of Slabs-on-Ground. American Concrete Institute.
ACI Committee 305. ACI 305R: Guide to Hot Weather Concreting. American Concrete Institute.
ACI Committee 301. ACI 301: Specifications for Concrete Construction. American Concrete Institute.
Neville, A. M. (2011). Properties of Concrete (5th ed.). Pearson Education.
Mehta, P. K., & Monteiro, P. J. M. (2014). Concrete: Microstructure, Properties, and Materials (4th ed.). McGraw-Hill Education.
Holt, E. E. (2001). Early Age Autogenous Shrinkage of Concrete. VTT Publications 446, Technical Research Centre of Finland.
Bažant, Z. P., & Najjar, L. J. (1972). Nonlinear water diffusion in nonsaturated concrete. Materials and Structures, 5(25), 3–20.